Hawsha Dhirta ee Dufanka Duugga ah Birta Ductile
Nidaamka soo-saarka soo-saarka caadiga ah ee birta duleelka, qiyaastii 10% kaarboon kaarboon ah ayaa guud ahaan loo isticmaalaa walxaha. Qodobkani wuxuu kaliya ka hadlayaa arrimaha qaarkood oo ay tahay in fiiro gaar ah loo yeesho habka wax soo saarka kadib markii la kordhiyo saamiga kaarboonka loo isticmaalo soosaarida birta duleelka ee foornada soosaarida. Marka loo eego wax soo saarka, qoraagu wuxuu soo bandhigayaa aragtidiisa u gaarka ah ee tixraaca asxaabta.
Xulashada lacagta
(1) Bir duug ah
Iskaraab loo adeegsaday soo saarista birta duleelka waa inay noqotaa kaarboon kaarboon ah. Waa inaysan ku jirin waxyaabo caqabad ku ah garaaf garaynta, sida chromium. Waa inaysan ku jirin waxyaabo ka kooban waxyaabo isku dhafan oo anti-spheroidizing ah. Kuus kuus ka sameysan bir duug ah waa inay ahaadaan ilaa 30% qaab jajab qaro weyn leh, oo si siman loo dhex dhigi karo foornada.
(2) Dib -u -hagaajiye
- Coke tayo sare leh. Sunta baaruuddu waa inay hooseysaa, uusku waa 60-80mm, wuxuuna leeyahay awood sare. Lama burburin karo ka dib marka la gubo.
- Pent Maska koronto Waxaa ugu fiican in la helo dherer cayiman si loo fududeeyo jarista birta la dhalaaliyay.
(3) Bir tuur
Waxaa badanaa loo isticmaalaa in lagu hagaajiyo kaarboonka birta dhalaashay. Rajey inaad isticmaasho birta doofaarka hoose ee baaruud-baaburka leh wC> 4%. Waxyaabaha ay ka kooban tahay silsiladda ku jirta birta doofaarka ayaa si ku habboon u sarreeya, iyo soo saarista birta birta ah ee loo yaqaan 'nodular iron iron' waxay noqon kartaa wax ka yar ferrosilicon.
(4) Sifeynta
Sroidroidizing agent iyo inoculant waxaa loo isticmaalaa si waafaqsan farsamooyinka dhaqameed, waxaana lagu go'aamiyaa iyadoo la raacayo xaaladaha dhabta ah ee warshad kasta.
Qosol
Habka dareeraha: Coke block + birta haraaga ah → koronto koronto → kororka heerkulka → soo jiida koke iyo koronto koronto → muunad iyo falanqeeyaan kaarboonka iron birta doofaarka → wax soo celinta → muunad iyo falanqeeyaan Si, Mn → kororka → ferromanganese + dheecaanka ferrosilicon → Cirbadeynta + spheroidization → daadinta.
Taxaddarrada inta lagu gudajiro howsha dhalaalintu waa sida soo socota:
- Qalabka coke-ka ayaa lagu rakibay salka foornada, ujeedku waa in la abuuro waqti dheer oo qoyaanka ah ee coke block birta dhalaashay. Qaddarka xinjiraha 'coke block' waa qiyaastii 5% duugga ah. Qiyaastii 50% duugga ah ayaa dhalaalay, kookaha waa in lagu daboolaa qashin dufan leh. Waxa kale oo suurtogal ah in la isticmaalo baloogyada korantada qashinka ee 60-80 mm halkii laga isticmaali lahaa coke oo lagu rakibo salka foornada sidii dib-u-habeyn, oo ay ku jirto maadadda baaruuddu ka hooseyso, taas oo faa'iido badan u leh helitaanka birta ductile tayo sare leh.
- Qiyaasta birta duugga ah ee la isticmaalay waxaa badanaa lagu go'aamiyaa waxtarka kororka kaarboonka. Soosaarayaasha bilaaba inay adeegsadaan habkan si ay u soo saaraan birta duleelka, qiyaastii 30% ayaa ka fiican. Ka dib hagaajinta waxtarka kororka kaarboonka, si tartiib tartiib ah u kordhi saamiga birta duugga ah. Isticmaalka xad-dhaafka ah ee birta duugga ah, haddii waxtarka kororka kaarboonku uusan sarreeynin, wuxuu saameyn ku yeelanayaa kaarboon-ka-silikoon u dhigma ee alaabada ugu dambeysa.
- Ka dib markii birta duugga ah la dhalaaliyo, geli usha korantada si aad si habboon ugu kordhiso heerkulka foornada oo aad u kordhiso waxtarka kaarboonka. Si kastaba ha noqotee, heerkulka foornada ayaa aad u sarreeya, taas oo kordhisa isticmaalka korontada sidoo kalena waxyeello u leh dahaarka foornada.
- Ka dib marka maadada kaarboon la qiyaaso inay sarreyso, soo qaado qashinka coke iyo koronto, iyo muunad oo falanqee waxyaabaha kaarboonka.
- Marka loo eego natiijooyinka falanqaynta, xisaabso qadarka birta doofaarka lagu daro iyo xaddiga birta dib loo warshadeeyay ee la isticmaalay.
- Go'aami in wadarta qadarka birta la shubay lagu samayn karo walxaha la cusbooneysiiyay iyadoo lagu saleynayo qiyaasta waxyaabaha ku jira silsiladda.
- Ka dib marka qalabka dhalaalaya dhalaaliyo, qaado muunad oo falanqee waxyaabaha ku jira Si, Mn iyo walxaha kale ee isku dhafan.
- Si sax ah u kordhi heerkulka birta la shubay, ku dar waxyaabaha isku dhafan sida ku xusan natiijooyinka falanqaynta, kuna dar ferrosilicon ka hor inta foornadu gaarin heerkulka foornada.
- Ferrosilicon waxaa loo dhalaaliyay xaalad la dhalaaliyay waxaana isla markiiba laga sii daayaa foornada.
- Sroidroidization, tallaalida, iyo daadinta waxaa loo sameeyaa sidii caadiga ahayd.
Xisaabinta qaabeynta qaab dhismeedka
Sidaan wada ognahay, sifooyinka farsamaysan ee birta ductile waxay inta badan kuxirantahay halabuurka kiimikada, heerka qaboojinta (as-cast iron iron) iyo geedi socodka daaweynta kuleylka. Isku-darka kiimikada waa sababta gudaha, asalka, iyo isbeddelka, ku dhowaad foornada kasta way ka duwan tahay. Sidaa darteed, waxaa lagama maarmaan ah in la xoojiyo ogaanshaha qaybaha kiimikada iyo in si taxaddar leh loo saxo, mana haboona in la qaato "waxsoosaarka saamiga go'an". Isku-darka kiimikada, kaarboon u dhiganta ayaa si gaar ah muhiim u ah. Gaar ahaan, macdanta birta ah ee loo yaqaan 'nodular cast iron' oo ay soo saaraan iyadoo la adeegsanayo birta duugga ah ee lacagta ugu badan ka qaadata, maxaa yeelay waxtarka kororka kaarboonka way adag tahay in la xakameeyo, kaarboonka u dhigmaana si aad ah ayuu u sarreeyaa, sidaa darteed waa in fiiro gaar ah la siiyaa sidii loo hagaajin lahaa kaarboon u dhigma.
- Xisaabi qadarka birta doofaarka lagu daray. Xisaabi qadarka birta doofaarka ah ee lagu daray iyadoo lagu saleynayo falanqaynta waxyaabaha kaarboon ka kooban. Xaqiiqdii, waa in la hagaajiyo kaarboon u dhiganta birta birta ee nodular si markaa kaarboon u dhiganta dhalaalka ay sameeyeen birta doofaarka iyo birta duugga ahi u gaadho kaarboonka u dhigma ee looga baahan yahay birta birta ah. duug ah oo lagu daray × (waxyaabaha loo baahan yahay ee kaarboonku ka kooban yahay ee birta birta ah ee falanqaynta maadada kaarboon) / (Kaarboonku ka kooban yahay birta doofaarka - Kaarboonka loo baahan yahay ee birta qanjidhada)
- Xisaabinta xaddiga lagu daray ee birta duugga ah ee dib loo warshadeeyay Kaarboon u dhiganta birta duugga ah ee dib loo warshadeeyay asal ahaan waa caadi, tirada lagu darayna ma badna. Sidaa darteed, ka dib marka birta dib loo kululeeyo lagu daro, kaarboonta ku jirta birta la shubay ee foornada oo dhan ayaa u qalma. birta lagu daray
- Qiyaasta waxa ku jira silikoonka Qaaciddada xisaabintu waa sida soo socota: Waxyaabaha loo yaqaan 'Silicon' ≈ ((birta duug ah + birta doofaarka + qaddarka dheeriga ah ee birta lagu shubo) content Waxyaabaha ay ka kooban tahay silikoon / wadarta guudba) × 100% ≤ Waxyaabaha ay ka kooban tahay silikoon ee birta dhalaalay asalka ah. waxa ku jira aad ayuu u sarreeyaa, ku dar qadar yar oo bir duug ah oo dib loo warshadeeyay, isticmaalna qadar isku mid ah birta doofaarka iyo duugga oo leh saamiga 9: 1 si aad uga dhigto wadarta lacagta.
- Xisaabinta Isugeynta Ferrosilicon Qaaciddada xisaabinta waa sida soo socota: Qaddarka ferrosilicon ee lagu daray = [wadarta guud ee lacagta charge (wadarta silsiladda loo baahan yahay ee maadada birta ah ee dufanka ku kordhay iyadoo la adeegsanayo tallaalka-lagu kordhiyay maadada silicon iyadoo la adeegsanayo spheroidization-analysis of silicon content)] / maadada silikoon ee ferrosilicon
- Qadarka manganese iyo walxaha kale ee alwaaxa lagu daray waxaa loo xisaabiyaa sida soo socota: Qaddarka birta daawaha ah ee lagu daray = wadarta guud ee lacag bixinta × (waxa loo baahan yahay ee ay ka kooban tahay maadada birta falanqaynta birta ah) oo lagu soo daray xisaabinta kor ku xusan.
Tani waa sababta oo ah birta birta ah ee loo yaqaan 'nodular cast iron' ayaa lagu dhalaaliyaa foornada kuleylka, iyo walxaha wax badan ma gubtaan, birta sidoo kale waa la gubaa ilaa xad. Haddii aad la kulanto duruufo gaar ah, waa inaad fiiro gaar ah u leedahay gubashada.
Tusaalaha dalabinta qaabeynta halabuurka:
- Iyadoo la adeegsanayo 1t foornada korantada ee korantada si loo soo saaro birta loo yaqaan 'pearlitic ductile iron QT800-2, culeyska tuurista waa 1000kg.
- "Isku-darka kiimikada xakamaynta waa: wC = 3.5%, wSi = 2.5%, wMn = 0.5%, wP <0.07%, wS <0.02%, wMg = 0.03% ~ 0.06%, wRE = 0.02% ~ 0.04%.
- Dib-u-dhaqaajinta ka dib, waxa kaarboonku ka kooban yahay "birta qashinka lagu shubay" ee foornada ku jirta waa 2.5%.
- Qaddarka birta doofaarka lagu daray = 300 × (3.5% -2.5%) / (4% -3.5%) = 600 (kg)
- Qadarka birta birta ah ee loo isticmaalo foornada = 1000-300-600 = 100 (kg)
- Qiyaasta maaddada silikoon = (300 × 0.3% + 600 × 1.8% + 100 × 2.5%) × 100% = 1.42%
- Haddii nuxurka silsiladda ee nodulizer uu yahay 0.6% iyo waxyaabaha ay ka kooban tahay silikon ee sunta sunta ahi ay tahay 0.4%, waxyaabaha ay ka kooban tahay silikon ee macdanta birta asalka u ah waa inay ahaataa 1.5%, taas oo ka sarreysa heerka lagu qiyaasay silsiladda. Tan awgeed, birta birta ee loo yaqaan 'Z18 cast iron' ayaa loo isticmaali karaa in lagu hagaajiyo kaarboon u dhiganta, birta dib loo shidayna waxaa loo isticmaali karaa in lagu sameeyo wadarta guud ee lacagta.
- Maaddada silikoonku waa 1.38% maadada manganese-na waa 0.15% ka hor inta aan foornada la sii deyn.
- Ferrosilicon ayaa lagu daray qaddarka = [1000 (2.5% -0.6% -0.4% -1.38%)] / 75% = 1.6kg
- Qaddarka Ferromanganese ee lagu daray = [1000 (0.5% -0.15%)] / 65% = 5.4kg
4. Gebogebada hadalka
Soo saarida foornada korontada ku shaqeysa, waxaan u isticmaalnaa bir duug ah si aan u soo saarno QT800-2, xooggu waa 800 ~ 1000MPa, dheereynta ayaa ka badan 4%.
Waqtigaan la joogo, waxaa suuqa ku jira bir aad u badan oo duug ah, birta doofaarku waa qaali, birta doofaarka oo tayo sare lehna waa ka sii yaraanaysaa. Sidaa darteed, waxaan soo jeedinaynaa in soosaarayaasha leh howlaha wax soo saarka birta ee loo yaqaan 'nodular cast cast' ay tixraaci karaan fikradda aan kor ku soo sheegnay iyo "beddelidda birta birta" si ay u soo saaraan birta birta ah ee nodular
Fadlan hayso isha iyo cinwaanka maqaalkan si dib loogu daabaco:Hawsha Dhirta ee Dufanka Duugga ah Birta Ductile
Minghe Shirkadda Die Casting waxaa ka go'an in ay soosaaraan oo ay bixiyaan Qaybo ka ridaya tayo iyo waxqabad sare (biraha qaybo ka ridaya dhiman kala duwan inta badan ka mid yihiin Khafiifa-Wall dhinta ridaya,Hot ridaya die Cast,Kursiga Qabow Die Casting), Adeeg Wareeg ah (Adeegga Tartanka Dhimashada,Qalabka Mashiinka,Samaynta Furka, Daaweynta Dusha sare) .Caadi kasta oo Aluminium ah shubitaan, magnesium ama Zamak / zinc shubida iyo shuruudaha kale ee shubanka ayaa lagu soo dhaweynayaa inaad nala soo xiriirto.
Iyada oo ay gacanta ku hayaan ISO9001 iyo TS 16949, dhammaan geeddi-socodyada waxaa lagu fuliyaa iyada oo loo marayo boqollaal mashiinno shub ah oo dhimanaya, mashiinnada 5-dhidibka, iyo tas-hiilaadka kale, oo ka bilaabma qarxiyayaal ilaa mashiinnada dharka lagu nadiifiyo ee Ultra Sonic.Minghe ma ahan oo keliya qalab casri ah laakiin sidoo kale waxay leedahay xirfadle koox injineero khibrad leh, wadayaal iyo kormeerayaal si niyada macaamiisha ay u noqoto mid run ah.
Soo saaraha qandaraasle ee shubka dhinta. Awoodda waxaa ka mid ah qaybaha qabow ee aluminium ee qaybaha shubista laga bilaabo 0.15 lbs. illaa 6 rodol, isbeddel deg deg ah oo la dejiyay, iyo qalabaynta. Adeegyada qiimaha lagu daro waxaa ka mid ah sifaynta, gariirka, qashin-qubka, xabbadda toogashada, ranjiyeynta, dahaadhka, dahaadhka, isku-ururinta, iyo qalabaynta. Qalabka lala shaqeeyay waxaa ka mid ah alloysyada sida 360, 380, 383, iyo 413.
Zinc wuxuu u dhintaa caawinta naqshadeynta / adeegyada injineernimada isku mar. Soo saaraha gaarka ah ee saxda saxda ah ee looxyada. Daarayaasha yar-yar, cast-yada u dhinta cadaadiska sare, jilayaasha caaryada badan-slide, shubka caaryada caadiga ah, cutubka dhinta iyo kuwa madaxa-bannaan ee loo dhinto iyo daloolka dahaarka saanlan ayaa la soo saari karaa. Jilayaasha waxaa lagu soo saari karaa dherer iyo ballac ilaa 24 gudaha. +/- 0.0005 gudaha. Dulqaad.
ISO 9001: soo saaraha shahaadada leh ee loo yaqaan 'cast cast magnesium', Awoodaha waxaa ka mid ah dhimista cadaadiska sare ee magnesium oo loo ridayo ilaa 2015 ton qol kulul & 200 ton oo qol qabow ah, naqshadeynta qalabka, nadiifinta, wax u sameynta, mashiinada, budada & dareeraha rinjiyeynta, QA buuxda oo leh awooda CMM , ururinta, baakadaha & gaarsiinta.
ITAF16949 la xaqiijiyay. Adeeg Dheeraad Dheeraad ah Ayaa Kujira maalgelinta maalgelinta,ciida ciid,Dabaaldeg Shaqo, Casting Foam Fost,Khadka Centrifugal,Dabka Vacuum Casting,Qaab Joogtada ah, Awoodda waxaa ka mid ah EDI, kaalmada injineernimada, qaabeynta adag iyo ka shaqeynta heerka labaad.
Warshadaha Kabka Qaybaha Daraasada Kiiska ee loogu talagalay: Gawaarida, Baaskiiladaha, Diyaaradaha, Qalabka muusikada, Biyaha, Qalabka indhaha, Dareemayaasha, Moodooyinka, Aaladaha elektarooniga ah, Xiritaanka, Saacadaha, Mashiinnada, Mashiinnada, Qalabka guryaha, Dahabka, Jigs, Telecom, Laydhka, Qalabka Caafimaadka, Qalabka Sawirka, Robotyo, farshaxanno, qalabka codka, Qalabka isboortiga, Qalabaynta, Caruurta iyo waxyaabo kale oo badan.
Maxaan kaa caawin karnaa inaad sameyso marka xigta?
Tag bogga hore ee loogu talagalay Shiinaha dhinta Casting
→Qeybaha kabkaOgow waxaan soo qabanay.
Tips Tilmaamaha Halaasiga ah ee Ku Saabsan Adeegyada Cast Cast
By Soo saaraha Minghe Die Casting | Qeybaha: Maqaallo waxtar leh |Waxyaabaha Tags: Casting Aluminium, Tuurista Zinc, Ridaya Magnesium, Qalitaanka Titanium, Qalabka birta ee birta, Naxaas naxaas ah,Raxaama Naxaas,Video Tuuraya,Taariikhda Shirkadda,Calaamadda Aluminum Die Casting | Faallooyinka Off